Stainless Steel 17-4PH (1.4542): Properties, Aging and Machining
Updated
17-4PH (1.4542, AISI 630, UNS S17400) is a martensitic precipitation-hardening stainless steel with about 17 % chromium, 4 % nickel and 4 % copper. A simple aging treatment at 480–620 °C gives about 930–1310 MPa or more tensile strength and 28–44 HRC hardness while keeping corrosion resistance close to 304.
17-4PH is a martensitic precipitation-hardening (PH) stainless steel containing about 15–17.5 % chromium, 3–5 % nickel, 3–5 % copper and a small amount of niobium. Its EN 10088 material number is 1.4542 (X5CrNiCuNb16-4), AISI type 630 and UNS S17400. It combines high strength, good corrosion resistance and a simple heat treatment with little distortion.
How precipitation hardening works
The steel is supplied in Condition A (solution annealed): the structure is martensitic and hardness moderate. After machining, the part is aged at a single temperature, usually 480–620 °C, for a few hours. During aging, fine copper-rich particles precipitate in the martensite and raise strength and hardness. Conditions are named after the aging temperature in degrees Fahrenheit: H900, H1025, H1075, H1150 and so on. The lower the temperature, the higher the hardness but the lower the toughness. See heat treatment.
Properties by condition
| Condition | Aging | Tensile strength Rm | Typical hardness |
|---|---|---|---|
| A (solution annealed) | – | ≈ 1000–1100 MPa | ≈ 30–38 HRC |
| H900 | ≈ 480 °C, 1 h | ≥ ≈ 1310 MPa | ≈ 40–47 HRC |
| H1025 | ≈ 550 °C, 4 h | ≥ ≈ 1070 MPa | ≈ 35–42 HRC |
| H1150 | ≈ 620 °C, 4 h | ≥ ≈ 930 MPa | ≈ 28–37 HRC |
| General property | Value |
|---|---|
| Density | ≈ 7.8 g/cm³ |
| Magnetism | magnetic (martensitic structure) |
| Corrosion resistance | similar to 304 in many environments |
| Machinability | moderate to difficult; easiest in Condition A or H1150 |
Values are typical minimum or indicative figures based on common specification requirements; exact limits depend on the standard and product form. For hardness conversions see hardness scales.
Machinability
17-4PH is usually placed in ISO group M (ISO material groups). Compared with 304/316, it is less gummy and work-hardens less, but its higher hardness requires more cutting force and wears tools faster. In Condition A hardness can reach about 38 HRC, so the softer H1150 condition is sometimes preferred for machining.
| Operation (coated carbide) | Vc, m/min (A / H1150) | Feed |
|---|---|---|
| Turning | 90–160 | f ≈ 0.1–0.25 mm/rev |
| Milling with an end mill | 60–120 | fz ≈ 0.03–0.08 mm |
| Drilling with a carbide drill | 35–70 | f ≈ 0.06–0.15 mm/rev |
These are typical starting values; the tool manufacturer's data takes priority. Reduce cutting speed further for H900 material. See cutting speed and RPM.
Practical tips
- Machine before aging (in Condition A) and, if needed, do only finish grinding or light finishing after aging.
- Allow for dimensional change. The material contracts slightly and fairly uniformly during aging; for precision parts this is accounted for in the stock allowance or verified with a trial aging run.
- Use rigid workholding, short tools and carbide with TiAlN or AlTiN coating (tool coatings).
- Provide generous coolant; use through-tool coolant for deep drilling.
- For threading hard material, thread milling is more reliable than tapping.
- H900 is more brittle and more sensitive to stress corrosion cracking; when toughness matters, H1025–H1150 is chosen.
Typical uses
Aerospace components, pump and compressor shafts, valve parts, marine equipment, oil and gas components, medical and surgical instruments, mould inserts that need corrosion resistance, and high-strength fasteners.
How to choose
- Corrosion resistance needed but loads are modest – 304 or 316 is sufficient.
- High strength and corrosion resistance together – 17-4PH.
- Maximum hardness and strength – H900; better toughness and stress corrosion resistance – H1150.
- If low weight and high specific strength matter most – consider titanium alloy Ti6Al4V.
Machining services for 17-4PH parts can be found or requested on the CNC Pasaulis marketplace.
Frequently asked questions
What do H900 and H1150 mean?
They are aging condition codes based on the aging temperature in degrees Fahrenheit (about 480 °C and 620 °C). H900 gives the highest strength and hardness, H1150 lower hardness but better toughness.
Is 17-4PH magnetic?
Yes. Its martensitic structure makes 17-4PH magnetic, unlike annealed austenitic grades 304 and 316.
When is the best time to machine 17-4PH?
Usually in Condition A before aging, because afterwards only a simple aging treatment is needed, without quenching or significant distortion. Sometimes it is machined in H1150 when that is the final condition.
Do part dimensions change during aging?
Yes, the material contracts slightly and fairly uniformly. For precision parts this is handled by leaving stock or running a trial aging cycle.
Is 17-4PH as corrosion resistant as 316?
In many environments its resistance is similar to 304, but in chloride environments 316 is usually superior.