HDPE and UHMW-PE (PE 1000): Properties and Machining

Updated

In short

HDPE and UHMW-PE are high-density and ultra-high-molecular-weight polyethylenes: light, practically non-absorbent and chemically resistant. UHMW-PE (PE 1000) offers outstanding wear and impact resistance; both are easy to cut but soft, so tight tolerances are harder to hold.

Polyethylene (PE) is a semi-crystalline thermoplastic whose properties depend strongly on density and molecular weight. Two grades dominate machined parts: HDPE (high-density polyethylene, also called PE 300 or PE-HD) and UHMW-PE (ultra-high-molecular-weight polyethylene, PE-UHMW or PE 1000). An intermediate grade, PE 500, is also used in industry.

Property comparison

PropertyHDPE (PE 300)UHMW-PE (PE 1000)
Density, g/cm³0.94–0.970.93–0.94
Tensile strength, MPa20–3020–40
Tensile modulus, GPaapprox. 0.8–1.2approx. 0.7–0.8
Melting pointapprox. 130–135 °Capprox. 130–135 °C
Continuous service temperatureapprox. −50 to +80 °Capprox. −150 to +80 °C
Moisture absorption< 0.01 %< 0.01 %
Wear resistanceGoodVery good
MachinabilityEasy, soft, burrsEasy, stringy chips, burrs

Values are indicative; check the supplier's data sheet for exact figures.

Typical applications

  • HDPE: cutting boards and food-processing parts, tank and container components, chemical equipment parts, protective panels, marine hardware.
  • UHMW-PE: conveyor guides and wear strips, chain guides, star wheels, wear plates, hopper and chute liners, slide pads for lifting equipment.

CNC machining tips

  • Tools: very sharp tools with a large positive rake and large chip gullets; plastic-specific single-flute end mills are ideal. A dull tool pushes and melts PE instead of cutting it.
  • Parameters: PE tolerates high cutting speeds and feeds; a typical starting value for milling with carbide is about 250–600 m/min with relatively high feed. The tool manufacturer's data takes priority.
  • Cooling: compressed air to clear chips. PE does not absorb water, so water-based coolant can also be used.
  • Workholding: the material is soft and slippery; hold large plates with a vacuum table or several evenly spaced clamps. Excessive clamping force distorts the blank.
  • Burrs: PE, and UHMW-PE in particular, leaves fuzz and burrs on edges – plan chamfers and a finishing pass with a sharp tool.

Accuracy and distortion

Polyethylene has a high coefficient of thermal expansion – about 150–200·10⁻⁶ 1/K – so a 1 m long part warming by 20 °C grows by roughly 3–4 mm. Sheets also contain internal stress and can bow when a lot of material is removed from one side. Tips:

  • remove material symmetrically from both faces;
  • allow expansion gaps and slotted fixing holes in long parts such as guide rails;
  • measure precision parts at room temperature after they have cooled;
  • a realistic tolerance is usually ±0.1–0.2 mm, tighter on small parts.

Turning and large blanks

HDPE and UHMW-PE rod is turned into rollers, bushings, star wheels and screw segments. Sharp aluminium or plastic inserts with a large positive rake are suitable. A typical starting feed for turning is about 0.1–0.5 mm/rev, and depth of cut can be large because cutting forces are low. The tool manufacturer's data takes priority. UHMW-PE chips are particularly tough and long – they wrap around the workpiece – so they must be controlled and cleared frequently.

Polyethylene sheet is produced in very large formats (for example 2–3 m wide and 4–6 m long), so long guide rails and liner plates require routers or milling machines with a large working area. Thanks to low density even large parts are light, but their high thermal expansion means they must be machined and measured at a stable temperature.

Joining and colours

Polyethylene is almost impossible to glue, so parts are joined with countersunk screws, rivets or welded by hot-air, extrusion or butt welding. In guide rails, screw heads must be countersunk deeper than the expected wear depth so they do not scratch the sliding product.

The food industry often uses coloured PE grades to separate zones (for example green, blue, red). Blue is used so that any fragment that accidentally enters a product is easy to spot. Colour and additives do not fundamentally change properties, but antistatic or UV-stabilised grades may differ in density and cost.

How to choose

Choose HDPE for a low-cost, chemically resistant, food-compatible and easy-to-machine material without heavy wear. Choose UHMW-PE when the part wears, takes impacts or works at very low temperatures. If you need more stiffness, precision or service above 80 °C, POM or PA6 are better.

Suitable polyethylene machining services can be found or requested on the CNC Pasaulis marketplace.

Frequently asked questions

What is the difference between PE 300, PE 500 and PE 1000?

The number broadly indicates molecular weight: PE 300 is HDPE, PE 1000 is UHMW-PE and PE 500 is an intermediate grade. Wear and impact resistance increase with molecular weight.

Why is UHMW-PE so wear resistant?

Its very long polymer chains give exceptional toughness and low friction. That is why it is used for conveyor guides, chain guides and liners.

Is polyethylene suitable for food contact?

Yes, HDPE and UHMW-PE grades meeting food-contact requirements are available. Check suitability in the supplier's documentation.

Why does an HDPE plate warp after milling?

Because of internal stress and asymmetric material removal. Remove material evenly from both sides and machine in several stages.

Can PE be glued?

PE bonds very poorly with ordinary adhesives due to its low surface energy. Mechanical fastening or welding is more common.