Aluminium 7075: High-Strength Alloy Properties and Machining

Updated

In short

7075 is a high-strength Al-Zn-Mg-Cu alloy with a tensile strength of about 500–570 MPa in T6, comparable to structural steel at almost one third of the density. It machines excellently but is not suitable for fusion welding and has lower corrosion resistance than the 6xxx series.

Aluminium 7075 is a 7xxx-series wrought aluminium alloy whose main alloying element is zinc, with additions of magnesium and copper. In the heat-treated condition it is one of the strongest widely available aluminium alloys. For this reason 7075 is used in aerospace, sports equipment, mould making and anywhere high strength at low weight is required.

Designations and composition

  • EN: EN AW-7075 (AlZn5.5MgCu), W.Nr. 3.4365
  • UNS: A97075
  • Typical composition: Zn 5.1–6.1 %, Mg 2.1–2.9 %, Cu 1.2–2.0 %, Cr 0.18–0.28 %.

Properties

Property7075 T6 / T6517075 T73 / T7351
Density~2.81 g/cm³~2.81 g/cm³
Tensile strength Rm~500–570 MPa~460–500 MPa
Yield strength Rp0.2~430–500 MPa~380–430 MPa
Hardness~140–160 HB~130–145 HB
Young's modulus~71–72 GPa~71–72 GPa
Thermal conductivity~130 W/(m·K)~150 W/(m·K)
MachinabilityVery good, short chipsVery good

Values are typical; minimum limits depend on thickness and standard (EN 485, EN 755). The T73 temper is over-aged to improve resistance to stress corrosion cracking at the cost of some strength.

Advantages and drawbacks

AdvantagesDrawbacks
Very high strength and strength-to-weight ratioNot suitable for fusion welding (hot cracking)
Excellent machinability and surface finishLower corrosion resistance than 5xxx and 6xxx
Less prone to built-up edge than soft alloysSusceptible to stress corrosion cracking in T6
Suitable for hard anodisingMore expensive than 6082

Machining tips

  • Tools. Carbide end mills with 2–3 flutes, polished flutes and a sharp edge. Being harder, 7075 produces shorter chips that break better than 6082.
  • Cutting data. Cutting speeds similar to or slightly below 6082 are typical. These are starting values; exact data comes from the tool manufacturer. See cutting speed and RPM and feed per tooth.
  • Residual stress. Thick plate is usually supplied as T651 or T7351; even so, removing a lot of material can cause distortion. Separate roughing, stress relaxation and finishing into distinct stages.
  • Surface finish. 7075 allows a very good finish; Ra 0.8–1.6 µm is common when milling with sharp tools. See surface roughness.
  • Coolant. Emulsion or MQL; the key is effective chip evacuation.

Stiffness and design considerations

When designing in 7075, remember that high strength does not mean high stiffness. Its Young's modulus (about 71 GPa) is almost the same as 6082, so switching from 6082 to 7075 makes a part stronger but not stiffer – with the same geometry, deflection stays similar. Only geometry increases stiffness: ribs, wall height and thickness. Second, 7075 is more notch-sensitive than softer alloys, so internal corner radii and smooth transitions are recommended, especially under fatigue loading. Third, threads in 7075 are stronger than in 6082, but threaded inserts are often used for frequently loaded joints. Prolonged exposure above roughly 100–150 °C starts to reduce T6 strength, so parts operating at elevated temperature should be designed with care.

Surface finishing

7075 can be anodised and hard anodised, but because of copper and zinc the colour is often less uniform than with the 6xxx series, and clear anodising may look slightly yellowish. If decorative appearance matters, test a sample first. See anodizing.

Typical applications

  • Aerospace structural parts, brackets and fittings.
  • Bicycle, climbing, shooting sport and motorsport components.
  • Plastic injection moulds and prototype tooling for short runs.
  • Robotics and automation parts where weight and stiffness matter.

When to choose 7075

Choose 7075 when 6082 or 6061 is not strong enough and steel is too heavy. If the part will be welded or permanently exposed to moisture or seawater, 6082 or 5083 is the better choice. For the best machinability in turning, consider 2xxx-series alloys. Machining services in 7075 can be found on the CNC Pasaulis marketplace.

Frequently asked questions

Is 7075 stronger than steel?

The tensile strength of 7075 T6 (about 500–570 MPa) exceeds S235 and is similar to S355, but its Young's modulus is about one third that of steel, so the part is more flexible.

Can 7075 be welded?

Fusion welding (TIG, MIG) is generally not suitable for 7075 because of hot cracking and loss of strength; bolted or riveted joints are used instead.

What is the difference between 7075 T6 and T651?

Mechanical properties are similar, but T651 is additionally stretched to reduce residual stress, so plates distort less during milling.

Does 7075 anodise well?

Yes, it can be anodised and hard anodised, although the colour is often less uniform than with 6xxx-series alloys.

What is the hardness of 7075?

In T6 condition 7075 typically has a hardness of about 140–160 HB.

Looking for someone to do this job? Find a manufacturer on the marketplace or post a request.

Services offered I need a service