Aluminium Anodizing: Types, Thickness, Colours and Drawing Callouts
Updated
Anodizing is an electrochemical process that grows a controlled layer of aluminium oxide on aluminium, improving corrosion and wear resistance and allowing the part to be coloured. The most common forms are sulphuric acid anodizing (about 5–25 µm) and hard anodizing (about 25–100 µm).
Anodizing (anodic oxidation) is an electrochemical surface treatment in which an aluminium part is made the anode in an electrolyte bath, forming a porous aluminium oxide (Al2O3) layer on its surface. Unlike paint or electroplated coatings, the oxide grows from the metal itself and is therefore integrally bonded.
Types of anodizing
A widely used classification is the US military specification MIL-A-8625 (Types I, II, III); in Europe decorative and protective anodizing is covered by ISO 7599 and hard anodizing by ISO 10074.
| Type | Electrolyte | Typical thickness | Properties and use |
|---|---|---|---|
| Type I (chromic) | Chromic acid | ~0.5–7.5 µm | Thin, minimal dimensional change; aerospace. Use of hexavalent chromium is restricted and being replaced by alternatives |
| Type II (sulphuric) | Sulphuric acid, room temperature | ~5–25 µm | Most common; corrosion resistance, dyeing, decorative |
| Type III (hard) | Sulphuric acid, low temperature, higher current density | ~25–100 µm (most often 25–50 µm) | High hardness and wear resistance, electrical insulation; darker natural colour |
Under ISO 7599 the decorative coating class is designated by thickness, e.g. AA10, AA15, AA20, AA25 (minimum average thickness in µm). Thicker layers (e.g. 20–25 µm) are generally recommended for outdoor exposure.
Dimensional change
The oxide layer grows roughly half into the metal and half outward. Each surface therefore grows by about half the coating thickness, and a diameter changes by about the full coating thickness.
| Coating thickness | Surface build-up (approx.) | Diameter change (approx.) |
|---|---|---|
| 10 µm | +5 µm | +10 µm (shaft) / −10 µm (bore) |
| 25 µm | +12.5 µm | +25 µm / −25 µm |
| 50 µm (hard) | +25 µm | +50 µm / −50 µm |
Exact ratios depend on alloy and process. This matters greatly for holes and threads with tight tolerances: they must be machined with an allowance or masked.
Colouring and sealing
- Dyeing – the porous oxide absorbs organic or inorganic dyes: black, red, blue, gold and others. Colour consistency depends on alloy and batch, so shades may vary slightly between batches.
- Electrolytic colouring – metal salts are deposited in the pores; bronze and black shades with good UV resistance, widely used in architecture.
- Sealing – after anodizing the pores are closed (hot water, nickel acetate or other methods). This greatly improves corrosion resistance and retains colour. Hard anodizing is sometimes left unsealed to maximise wear resistance.
Alloy suitability
| Alloy group | Suitability |
|---|---|
| 6xxx (e.g. 6060, 6061, 6082) | Very good; the most common choice |
| 5xxx (e.g. 5754, 5083) | Good |
| 7xxx (e.g. 7075) | Good, but colour may be less uniform |
| 2xxx (e.g. 2024, 2007) | Limited – copper gives a thinner, less resistant layer |
| High-silicon casting alloys | Limited – dark, uneven coating |
More on alloys in aluminium alloys.
How to specify on a drawing
- Process type and standard (e.g. sulphuric anodizing per ISO 7599 or MIL-A-8625 Type II).
- Coating thickness or class (e.g. 15–20 µm, AA15).
- Colour and whether sealing is required.
- Whether dimensions apply before or after anodizing.
- Surfaces to be masked (threads, electrical contact points, fitting surfaces).
- Racking points – where a contact mark may remain.
Practical tips
- Sharp edges coat poorly – provide at least small chamfers or radii.
- An anodized surface is electrically non-conductive, so grounding points must be masked.
- Surface roughness and machining marks remain visible through the coating; for a matte look, bead blasting or etching is used before anodizing.
Anodizing and aluminium machining services can be found or requested on the CNC Pasaulis marketplace.
Frequently asked questions
What is the difference between standard and hard anodizing?
Standard (Type II) anodizing forms about 5–25 µm, suitable for corrosion protection and colour. Hard (Type III) forms about 25–100 µm with much higher wear resistance.
How much does anodizing change dimensions?
About half the coating thickness per surface, so a diameter changes by roughly the full coating thickness.
Can any aluminium be anodized?
Most alloys can, with the 6xxx series best suited. Alloys high in copper or silicon give poorer, uneven coatings.
Is an anodized coating electrically conductive?
No, aluminium oxide is an insulator. Contact points must be masked or machined after anodizing.
What is anodize sealing?
Closing the pores after anodizing, often with hot water or nickel acetate. It improves corrosion resistance and preserves colour.
Looking for someone to do this job? Find a manufacturer on the marketplace or post a request.