Heat Treatment of Metals: Hardening, Tempering, Case Hardening and Nitriding
Updated
Heat treatment is the controlled heating and cooling of metal to change its structure and properties: hardness, strength, ductility and residual stress. For CNC parts the most common processes are hardening and tempering, case hardening, nitriding, induction hardening, stress relieving and age hardening of aluminium alloys (T6).
Heat treatment is a group of processes in which metal is heated to a set temperature, held and cooled at a defined rate to obtain the required microstructure and properties. It determines whether a part will be hard and wear-resistant or ductile and easy to machine.
Main heat treatments for steel
| Process | Purpose | Typical result |
|---|---|---|
| Soft annealing | Soften, improve machinability | Low hardness, good formability |
| Normalising | Homogenise and refine the structure | Uniform properties after forging or welding |
| Stress relieving | Reduce residual stress after welding or roughing | Less distortion in finishing; hardness barely changes |
| Hardening and tempering (+QT) | Increase strength and hardness while keeping toughness | E.g. 42CrMo4 +QT – typically ~28–34 HRC depending on section |
| Through hardening to high hardness | Wear resistance | Tool steels ~55–62 HRC |
| Carburising (case hardening) | Hard surface, tough core | Surface ~58–62 HRC, case often 0.5–1.5 mm |
| Nitriding | Hard, wear- and fatigue-resistant surface with minimal distortion | Case ~0.1–0.6 mm, process ~500–570 °C |
| Induction hardening | Local surface hardening | Case ~0.5–5 mm, only where needed |
Exact temperatures and hardness values depend on steel grade and section size; they are set according to material standards (e.g. the EN ISO 683 series) and the heat treater's experience. Hardness units are explained in hardness scales.
Typical steel grades
| Steel (EN) | Use | Typical heat treatment |
|---|---|---|
| C45 (1.0503) | Shafts, axles | Quench and temper or induction hardening |
| 42CrMo4 (1.7225) | Highly loaded parts, shafts, bolts | Quench and temper (+QT), induction hardening, nitriding |
| 16MnCr5 (1.7131) | Gears, pins | Carburising and hardening |
| X153CrMoV12 (1.2379) | Dies, blades | Hardening to ~58–62 HRC |
| 40CrMnMo7 (1.2311) | Plastic moulds | Often supplied pre-hardened (~28–34 HRC) |
Heat treatment of aluminium alloys
Heat-treatable aluminium alloys (2xxx, 6xxx, 7xxx) are solution treated, quenched and artificially aged. Tempers are designated per EN 515: e.g. T6 – solution treated and artificially aged; T651 – additionally stretched to relieve stress. More in aluminium alloys. Austenitic stainless steels cannot be hardened by quenching; they are solution annealed.
Heat treatment and CNC machining
- Sequence: a part is often rough machined, heat treated and then finish machined or ground. Quenched and tempered steel (~28–34 HRC) generally still mills and turns well.
- Distortion: hardening distorts parts and changes dimensions, so stock is left and precision surfaces are finished after hardening.
- Hard workpieces: material above ~45–50 HRC can be milled only with special tools; above ~60 HRC it is usually ground or machined by EDM.
- Stop-off: areas that must remain soft (e.g. for later threading) can be protected with stop-off paste or copper plating during carburising.
- Scale: heating in air forms oxide scale; vacuum or protective atmosphere processes reduce it.
What to specify on the drawing
- Process and required hardness with tolerance (e.g. 58–62 HRC).
- Case depth and its definition (e.g. effective case depth CHD per ISO 18203 at a specified hardness).
- Measurement location and method.
- Areas that must not be hardened.
- Whether a certificate or report is required.
Drawing requirements are discussed further in technical drawings for CNC machining. Heat treatment and machining services can be found or requested on the CNC Pasaulis marketplace.
Frequently asked questions
What is the difference between hardening and quench-and-temper?
Quench and temper is hardening followed by high-temperature tempering, giving strength and toughness (e.g. ~28–34 HRC). Hardening with low tempering gives high hardness (often above 55 HRC).
When should nitriding be chosen over carburising?
When minimal distortion is required, since nitriding takes place at lower temperature without quenching. The case is thinner than with carburising.
Can a part be machined after hardening?
Yes, but it is harder: quenched and tempered steel can be milled and turned, while very hard steel is usually ground or EDM machined.
What does aluminium temper T6 mean?
The alloy has been solution treated, quenched and artificially aged to achieve high strength.
Why do parts distort during hardening?
Because of temperature gradients, phase transformations and residual stresses. Stock is therefore left for finish machining.
Looking for someone to do this job? Find a manufacturer on the marketplace or post a request.