Galvanizing and Zinc Plating: Hot-Dip vs Electroplated Zinc
Updated
Zinc coating protects steel from corrosion both as a barrier and as a sacrificial (cathodic) anode. Hot-dip galvanizing (EN ISO 1461) gives a thick coating, typically 45–85 µm or more, for structures, while zinc electroplating (ISO 2081) gives a thin, precise 5–25 µm coating for small parts and fasteners.
Zinc coating is the application of zinc to steel or cast iron to protect it from corrosion. Zinc is more active than iron, so even if the coating is damaged, the zinc corrodes first and protects the steel cathodically. Two methods dominate in industry: hot-dip galvanizing and zinc electroplating.
Comparison
| Property | Hot-dip galvanizing | Zinc electroplating |
|---|---|---|
| Process | Immersion in molten zinc (~450 °C) | Electrolytic deposition from an aqueous solution |
| Standard | EN ISO 1461 (articles), EN ISO 10684 (fasteners) | ISO 2081 (+ ISO 4042 for fasteners) |
| Typical thickness | ~45–85 µm and more, depending on steel thickness | ~5–25 µm (often 8–12 µm) |
| Appearance | Grey, sometimes spangled, rougher | Smooth, bright; colour set by passivate |
| Dimensional accuracy | Low – uneven thickness, possible drips | High – suitable for threads and precise features |
| Corrosion protection | Long-term outdoors | Moderate; indoor and mild outdoor conditions |
| Typical use | Steel structures, fencing, frames, supports | Bolts, washers, small turned and milled parts, sheet metal parts |
Hot-dip galvanizing
The article is degreased, pickled in acid, fluxed and dipped in molten zinc. Zinc reacts with the steel to form iron–zinc alloy layers with pure zinc on top. EN ISO 1461 specifies minimum mean coating thickness by steel thickness – for example, 85 µm minimum mean for steel thicker than 6 mm.
- Steel chemistry – silicon and phosphorus content strongly affects coating thickness and appearance (the Sandelin effect).
- Design – closed hollow sections need vent and drain holes, otherwise there is a risk of explosion or uncoated areas.
- Distortion – thin sheet and asymmetric welded structures may distort due to temperature.
- Threads – internal threads are often re-tapped after galvanizing, and fasteners use special tolerance classes.
Zinc electroplating
Parts are degreased, activated and plated with zinc or a zinc alloy (e.g. zinc–nickel, zinc–iron) in an electrolyte bath. Small parts are barrel plated and larger ones rack plated. After plating a passivate (conversion coating) is applied, which greatly increases corrosion resistance.
| Passivate | Appearance | Notes |
|---|---|---|
| Trivalent clear / blue | Silvery, bluish | Most common, free of hexavalent chromium |
| Trivalent thick-film (iridescent) | Iridescent | Better protection |
| Black passivate | Black | Often with an additional sealer |
Hexavalent chromium (yellow) passivates have been replaced by trivalent ones in many EU applications under RoHS, ELV and REACH. Corrosion resistance is often assessed by neutral salt spray testing (ISO 9227), with requirements stated in hours to white or red rust.
Hydrogen embrittlement
During electroplating, hydrogen can diffuse into high-strength steel and cause brittle fracture. For high hardness (typically above ~31–39 HRC, or property class 10.9 and higher) a baking treatment after plating is applied, or other coatings (e.g. zinc flake) are chosen. See hardness scales.
What to specify on the drawing
- Process and standard (e.g. zinc electroplating per ISO 2081, Fe/Zn 8, with trivalent passivate).
- Minimum thickness and required salt spray resistance if relevant.
- Whether dimensions apply before or after coating; thread tolerances (see metric threads).
- Whether hydrogen embrittlement relief baking is required.
Stainless steel does not need zinc coating – it is passivated instead. Paint systems over zinc are described in powder coating. Zinc coating services can be found or requested on the CNC Pasaulis marketplace.
Frequently asked questions
What is the difference between hot-dip galvanizing and zinc plating?
Hot-dip galvanizing forms a thick coating (often 45–85 µm or more) by dipping in molten zinc. Zinc plating forms a thin (5–25 µm), precise electrolytic coating.
Can threaded parts be hot-dip galvanized?
Yes, but internal threads often need re-tapping and external threads use special tolerance classes.
What is passivation after zinc plating?
A thin conversion coating on the zinc that greatly increases corrosion resistance. Trivalent chromium passivates are most common today.
What is hydrogen embrittlement?
Brittleness of high-strength steel caused by hydrogen absorbed during electroplating. It is reduced by baking soon after plating.
How long does hot-dip galvanizing last?
It depends on coating thickness and environmental corrosivity per ISO 9223 and ISO 14713. In low-corrosivity environments protection can last decades.
Looking for someone to do this job? Find a manufacturer on the marketplace or post a request.
Services offered I need a service