Hardness Scales HRC, HB and HV: Testing and Approximate Conversion
Updated
Metal hardness is most often measured with the Rockwell (HRC, HRB, ISO 6508), Brinell (HBW, ISO 6506) and Vickers (HV, ISO 6507) methods. Each uses a different indenter and load, so values can only be converted approximately using ISO 18265 or ASTM E140 tables. In CNC machining, hardness determines the tool material, cutting speed and whether a part is machined before or after heat treatment.
Hardness is a material's resistance to local plastic deformation when a harder indenter is pressed into its surface. It is the quickest and cheapest mechanical test, so it is used to verify material condition, heat-treatment results and machinability. The main scales for metals are standardised: Rockwell – ISO 6508, Brinell – ISO 6506, Vickers – ISO 6507. Plastics are measured with the Shore method (ISO 868), which is not covered here.
Comparison of methods
| Method | Standard | Indenter | Typical load | Typical use |
|---|---|---|---|---|
| Rockwell C (HRC) | ISO 6508-1 | Diamond cone 120° | 1471 N (150 kgf) | Hardened steels, ~20–70 HRC |
| Rockwell B (HRB) | ISO 6508-1 | Ball 1/16″ (1.5875 mm) | 980.7 N (100 kgf) | Soft steels, brass, aluminium |
| Brinell (HBW) | ISO 6506-1 | Carbide ball, usually 10 mm | 29.42 kN (3000 kgf) for steel | Cast iron, annealed and quenched-and-tempered steels, castings, up to 650 HBW |
| Vickers (HV) | ISO 6507-1 | Diamond pyramid 136° | 0.098 N to 980.7 N (e.g. HV10 = 98.07 N) | Full hardness range, thin coatings, case-hardened layers |
How the values are calculated
Vickers: the mean diagonal of the indentation d (mm) is measured and HV = 0.1891 × F / d², with F in newtons. Example: HV10 test (F = 98.07 N), d = 0.25 mm → HV = 0.1891 × 98.07 / 0.0625 ≈ 297 HV10.
Brinell: the indentation diameter d is measured and HBW = 0.102 × 2F / (π × D × (D − √(D² − d²))), where D is the ball diameter. Example: D = 10 mm, F = 29,420 N, d = 4.0 mm → D − √(100 − 16) = 10 − 9.165 = 0.835; HBW = 0.102 × 58,840 / (π × 10 × 0.835) ≈ 229 HBW.
Rockwell: instead of the indentation size, the permanent depth of penetration after removal of the major load is measured. The value is read directly from the instrument, which makes the method fast and well suited to production inspection.
Designation
58 HRC– Rockwell C scale.230 HBW 10/3000– Brinell, 10 mm carbide ball, 3000 kgf load.450 HV10– Vickers, 10 kgf (98.07 N) load.
Approximate conversion table (steel)
The table gives approximate values for non-alloy and low-alloy steels based on ISO 18265 / ASTM E140 type tables. Conversion depends on the material and its condition, so acceptance testing must use the method specified on the drawing.
| HRC | HV | HBW (approx.) | Rm, MPa (approx.) |
|---|---|---|---|
| 20 | 238 | 226 | ~770 |
| 25 | 266 | 253 | ~860 |
| 30 | 302 | 286 | ~960 |
| 35 | 345 | 327 | ~1100 |
| 40 | 392 | 371 | ~1250 |
| 45 | 446 | 421 | ~1450 |
| 50 | 513 | 481 | ~1650 |
| 55 | 595 | – | – |
| 60 | 697 | – | – |
| 65 | 832 | – | – |
For steels the approximate relationship Rm ≈ 3.3…3.5 × HB (MPa) applies. Above roughly 50 HRC the Brinell method is not used and strength conversion becomes unreliable.
Hardness and machinability
| Material and condition | Typical hardness | Machining note |
|---|---|---|
| Aluminium alloy 6082-T6 | ~90–100 HB | Easy to machine, ISO group N |
| Structural steel S355 | ~150–190 HB | ISO group P |
| Stainless steel 304/316 | ~150–215 HB | Work-hardens, ISO group M |
| 42CrMo4, quenched and tempered | ~28–36 HRC | Coated carbide |
| Hardened tool steel | ~55–62 HRC | Hard machining, ISO group H (CBN, ceramics, special carbide grades) |
See ISO material groups for more on the classification, and the cutting data tables for starting cutting values.
Practical tips
- Specify hardness on the drawing with the method and a range, e.g.
58–62 HRC, rather than a single value. - Where both high accuracy and high hardness are required, the part is usually machined before heat treatment with a stock allowance, then ground or hard-milled after hardening.
- For thin layers (case hardening, nitriding) use low-load Vickers and specify the effective case depth.
- Converted values (e.g. HB from HRC) are indicative only and should not be used for acceptance.
When requesting a quote on the CNC Pasaulis marketplace, stating the stock hardness helps the manufacturer estimate machining time and tooling cost more accurately.
Frequently asked questions
Can HRC be converted exactly to HB?
No, only approximately. Conversion tables (ISO 18265, ASTM E140) are empirical and valid for specific material groups, so the result is indicative.
From what hardness is machining considered hard machining?
Typically from about 45 HRC upwards. Such materials belong to ISO group H and need special carbide, ceramic or CBN tools.
Why is Brinell not used for hardened steel?
The carbide ball in ISO 6506 is limited to 650 HBW. Harder materials are tested with Rockwell C or Vickers.
Which method suits a thin coating or case?
Low-load Vickers (microhardness, e.g. HV0.1–HV1), because the small indentation does not punch through the layer.
How can steel strength be estimated from hardness?
Approximately Rm ≈ 3.3–3.5 × HB in MPa. This is only an estimate; actual strength is determined by a tensile test.
Looking for someone to do this job? Find a manufacturer on the marketplace or post a request.