PMMA (Acrylic): Properties and Machining

Updated

In short

PMMA (polymethyl methacrylate, acrylic) is a clear, hard but brittle thermoplastic that transmits about 92 % of visible light. It mills and engraves well, but is sensitive to internal stress, cracking and overheating, so it needs sharp tools and careful drilling.

PMMA (polymethyl methacrylate), commonly called acrylic or acrylic glass, is an amorphous transparent thermoplastic. It transmits about 92 % of visible light and has good UV and weather resistance, but is more brittle than polycarbonate. CNC machining of PMMA produces guards, display windows, light guides, signage and prototypes.

Cast vs extruded PMMA

  • Cast PMMA (GS) – higher molecular weight and lower internal stress; mills and engraves better and is less prone to melting and cracking. Recommended for CNC machining.
  • Extruded PMMA (XT) – cheaper with tighter thickness tolerance, but more internal stress; melts and gums up tools more easily and cracks more readily.

Key properties

PropertyTypical value
Density1.18–1.19 g/cm³
Tensile strength60–80 MPa
Tensile modulusapprox. 3.0–3.3 GPa
Light transmission (3 mm)approx. 92 %
Glass transition temperatureapprox. 105–110 °C
Continuous service temperatureapprox. −40 to +70…80 °C
Thermal expansionapprox. 70·10⁻⁶ 1/K
MachinabilityGood; sensitive to heat and cracking

Values are indicative; see the supplier's data sheet for exact figures.

Typical applications

  • Machine guards and inspection windows.
  • Light guides, diffusers and luminaire parts.
  • Sign letters, displays and exhibition elements.
  • Transparent prototypes, microfluidic and laboratory parts.

CNC milling tips

  • Tools: sharp, polished single-flute or two-flute cutters for plastics with large chip gullets. A polished edge gives a clearer cut surface.
  • Chip load: must be sufficient – too little feed at high RPM rubs the material, which melts and welds to the tool.
  • Parameters: typical starting values for a 6 mm single-flute cutter are 16,000–24,000 rpm with fz about 0.05–0.15 mm. The tool manufacturer's data takes priority; see cutting speed and RPM for the calculation.
  • Cooling: compressed air or air/fluid mist. Avoid solvent-containing fluids and oils, which can cause stress cracking (crazing).
  • Workholding: vacuum table or double-sided tape for thin sheet; avoid point clamps that induce stress.

Drilling and threading

Standard metal twist drills tend to grab in PMMA and chip the exit side. Use drills with a dubbed-off (zero or near-zero) rake or dedicated plastic drills, reduce feed before breakthrough and support the workpiece underneath. Threads in PMMA should be coarse, or use threaded inserts – fine threads break easily.

Surface finishing

Milled edges can be made clear by polishing with compounds, by flame polishing (cast PMMA only, risky due to stress) or by diamond tooling. For precision or bonded parts, annealing after machining (for example several hours at around 80 °C, following the producer's instructions) reduces internal stress and cracking risk.

Engraving and 3D milling

Cast PMMA is one of the most popular materials for CNC engraving. When engraving with V-bits or tapered cutters, the milled surface is matte and stands out in the clear sheet; when edge-lit it glows, which is how illuminated signs and lettering are made. Engraving uses small depths of cut (typically 0.1–0.5 mm per pass) and high spindle speeds. For 3D reliefs and lens shapes, ball-nose end mills with a small stepover are used, followed by polishing to clarity.

Extruded PMMA tends to melt during engraving and leave a messy edge, so it is less suitable for decorative work.

Bonding and secondary operations

PMMA parts are usually joined with solvent cements, which dissolve the surface and weld the parts. Such joints require smooth, accurate and stress-free edges – a milled edge should be annealed, otherwise the solvent in the cement causes fine cracks around the joint. PMMA can also be line-bent by heating to about 150–170 °C, but bend lines should not contain milled grooves that concentrate stress.

Clean PMMA with water and mild detergent; alcohol, acetone and many cleaners cause surface crazing. Leave the protective film on during machining and remove it only before assembly.

How to choose

Choose cast PMMA for CNC machining and engraving. Extruded sheet suits simple cutting and bending where cost and thickness tolerance matter. If the part will see impacts, consider polycarbonate (PC), which is far tougher but less scratch resistant.

Suitable PMMA machining services can be found or requested on the CNC Pasaulis marketplace.

Frequently asked questions

What is the difference between cast and extruded acrylic?

Cast PMMA has lower internal stress and higher molecular weight, so it mills and engraves better. Extruded sheet is cheaper with tighter thickness tolerance, but melts and cracks more easily during machining.

Why does acrylic melt when milling?

Usually because feed is too low at high RPM or the tool is dull, so it rubs instead of cutting. Increase the feed, use a sharp single-flute cutter and blow air on the cut.

How do I get a clear milled edge?

Use a sharp polished or diamond tool with a light finishing pass, then polish with compound. Flame polishing is only suitable for cast PMMA and can cause cracking.

Why do cracks appear around holes?

They are caused by internal stress, an unsuitable drill, or solvents and oils. Use plastic drills, avoid aggressive fluids and anneal the part if needed.

What temperature can PMMA withstand?

Continuous service is typically up to about 70–80 °C. The glass transition is about 105–110 °C, above which the material softens.