Carbon Steel C45 (1.0503): Properties, Heat Treatment and Machining

Updated

In short

C45 (1.0503) is a medium-carbon (about 0.45 % C) non-alloy steel to EN 10083-2, roughly equivalent to AISI 1045. It machines well, can be quenched and tempered or induction surface-hardened, and is widely used for shafts, axles, gears and pins.

C45 is a non-alloy medium-carbon steel for quenching and tempering, specified in EN 10083-2. Its material number is 1.0503 and its carbon content is 0.42–0.50 %. It is one of the most versatile steels in machine building: reasonably strong, inexpensive and easy to turn and mill.

Designation and equivalents

  • EN: C45 (1.0503); variants C45E (1.1191, restricted sulphur) and C45R (1.1201, controlled sulphur for better machinability).
  • Old DIN: C45, Ck45 (≈ C45E).
  • AISI/SAE: ≈ 1045; UNS: ≈ G10450.

These equivalents are approximate – composition limits differ slightly, so check the mill certificate for critical parts. See material designation equivalents.

Properties

PropertyNormalized (+N)Quenched and tempered (+QT)
Density≈ 7.85 g/cm³≈ 7.85 g/cm³
Tensile strength Rm≈ 580–700 MPa≈ 630–850 MPa (depends on diameter)
Yield strength≈ 305–340 MPa≈ 370–490 MPa
Typical hardness≈ 170–210 HB≈ 200–250 HB
Induction-hardened surface≈ 50–58 HRC
Machinabilitygood; best in annealed or normalized condition

Larger bars harden only to a limited depth, so the strength in the +QT condition decreases with increasing diameter. For hardness conversions see hardness scales.

Heat treatment

C45 is hardened by heating to about 820–860 °C and quenching in water or oil, then tempered at 550–660 °C when toughness is required. Because of its limited hardenability, it is most often used for induction or flame surface hardening: bearing seats on shafts or gear teeth become hard while the core stays tough. Water quenching carries a risk of cracking at sharp corners and holes, so designs should include radii. See heat treatment.

Machinability

C45 belongs to ISO group P (ISO material groups). Compared with S235 it is less gummy, chips break more easily and the finished surface is cleaner. Normalized or annealed stock machines most easily; +QT material needs lower cutting speeds. Surface-hardened zones (50+ HRC) can only be machined by grinding or hard turning with CBN inserts.

Operation (coated carbide)Vc, m/minFeed
Turning, roughing160–250f ≈ 0.2–0.4 mm/rev
Turning, finishing200–300f ≈ 0.05–0.15 mm/rev
Milling with an end mill120–220fz ≈ 0.05–0.12 mm
Drilling with a carbide drill70–110f ≈ 0.1–0.25 mm/rev

These are typical starting values for normalized steel; the tool manufacturer's data takes priority. For calculations see cutting speed and RPM.

Practical tips

  • Coated carbide grades in the P15–P25 range (e.g. TiAlN or TiCN coatings) are a good choice; see tool coatings.
  • If the part will be hardened, machine it beforehand and leave 0.2–0.5 mm grinding stock on critical surfaces.
  • Cold-drawn bar (+C) contains residual stress – long, slender shafts can bend after keyway milling.
  • Use tapping oil or emulsion when threading; C45 taps without particular difficulty.
  • The steel rusts – oil, black-oxide or paint parts after machining.

Typical uses

Shafts, axles, pins, bolts, gears, sprockets, couplings, clutch parts, hydraulic cylinder rods (often chrome-plated), tool holders and general machine parts that need more strength than structural steel. When higher strength in large sections or better impact toughness is required, alloy steel 42CrMo4 is used.

How to choose

  1. Static loads, welding – S235/S355 is sufficient.
  2. Shafts and parts needing a hard surface at an affordable price – C45 with induction hardening.
  3. Large cross-sections, fluctuating or impact loads – 42CrMo4.

Turning and milling services for C45 parts can be found or requested on the CNC Pasaulis marketplace.

Frequently asked questions

Are C45 and AISI 1045 the same steel?

They are close equivalents with similar carbon content, but composition limits and test requirements differ slightly, so verify the certificate for critical parts.

What hardness can C45 reach when hardened?

Induction or flame-hardened surfaces typically reach about 50–58 HRC. Through-hardening is limited by the steel's modest hardenability.

Can C45 be welded?

Yes, but because of the higher carbon content it requires preheating and slow cooling; otherwise cracks may form in the heat-affected zone.

What is the difference between C45 and C45E?

C45E (1.1191) has tighter limits on sulphur and phosphorus, making it cleaner and better suited to hardening. C45R has controlled sulphur that improves machinability.

In which condition is C45 easiest to machine?

Normalized or annealed C45 machines most easily; quenched and tempered stock needs lower cutting speeds, and surface-hardened zones need grinding or CBN tools.

Looking for someone to do this job? Find a manufacturer on the marketplace or post a request.

Services offered I need a service