PTFE (Teflon): Properties and Machining

Updated

In short

PTFE (polytetrafluoroethylene) is a fluoropolymer resistant to almost all chemicals, usable from −200 to +260 °C and with a very low friction coefficient. It is soft and easy to cut, but high thermal expansion, creep and burrs make tight tolerances difficult to hold.

PTFE (polytetrafluoroethylene, widely known by the trade name Teflon) is a fluoropolymer with one of the best chemical resistances and lowest friction coefficients of any engineering material. PTFE cannot be processed by conventional melt moulding: semi-finished products are made by compressing and sintering powder, and are supplied as rod, sheet, tube and billets that are then CNC machined.

Key properties

PropertyTypical value (unfilled PTFE)
Density2.14–2.20 g/cm³
Tensile strength20–35 MPa
Tensile modulusapprox. 0.4–0.7 GPa
Service temperatureapprox. −200 to +260 °C
Melting pointapprox. 327 °C
Friction coefficientapprox. 0.05–0.10 (dry, against steel)
Thermal expansionapprox. 100–200·10⁻⁶ 1/K, non-linear
MachinabilityEasy to cut, hard to hold dimensions

Values are indicative; check the supplier's data sheet for exact figures.

Filled grades

Pure PTFE is soft and prone to creep (cold flow under sustained load). Fillers are added to improve this:

  • Glass fibre (15–25 %) – less creep and wear, more abrasive on tools.
  • Carbon / graphite – better thermal conductivity and wear resistance.
  • Bronze (approx. 40–60 %) – highest load and wear resistance, lower chemical resistance.
  • MoS₂ – lower friction and wear in dry sliding.

Typical applications

  • Seals, gaskets, piston rings and valve seats.
  • Slide plates and bearing pads, bushings.
  • Chemical and pharmaceutical equipment parts, laboratory equipment.
  • High-frequency electrical insulators.

CNC machining tips

  • Tools: very sharp, polished carbide tools with a large positive rake; plastic-specific single-flute end mills work well. Use diamond-coated tools for filled grades.
  • Workholding: cutting forces are low, so clamp gently – excessive pressure deforms PTFE and dimensions change after release.
  • Cutting speed: a typical starting value for milling with carbide is about 150–400 m/min; the tool manufacturer's data takes priority.
  • Cooling: recommended, because PTFE conducts heat poorly and expands strongly. Use water-based coolant or compressed air.
  • Burrs: PTFE leaves soft burrs; finish passes need a sharp tool and a small, but not too small, depth of cut.
  • Safety: above about 400 °C PTFE decomposes and releases toxic fumes. Normal machining does not reach this, but avoid frictional overheating and do not smoke in the work area.

Accuracy and measurement

At around 19 °C PTFE undergoes a crystalline phase transition with a sudden volume change of about 1 %. Parts machined and measured at different temperatures may therefore differ by several hundredths of a millimetre. For precision parts, machine and measure at a stable temperature such as 23 °C; a realistic tolerance is usually ±0.05–0.1 mm, depending on size.

Turning and seals

A large share of PTFE parts – seal rings, gaskets and valve seats – is turned from rod or tube. Use very sharp inserts with a large positive rake and polished face; aluminium geometries work well. A typical starting feed is about 0.1–0.25 mm/rev, lower for finishing to achieve the surface roughness needed on sealing faces. The tool manufacturer's data takes priority. Chips form long, tough ribbons that must be guided away from the workpiece.

Thin-walled rings deform easily in the chuck, so soft bored jaws, expanding mandrels or vacuum holding are used. The part is often parted off the bar only after all surfaces have been machined.

Holes and threads

When drilling PTFE, the hole often closes up slightly after the drill is withdrawn – becoming a little smaller than the drill diameter – because the material recovers elastically. For precise holes, reaming or helical interpolation milling is used. Threads in PTFE are weak and creep, so loaded joints use metal threaded inserts or through-bolts. Filled grades (especially glass and bronze filled) machine more like abrasive composites and require wear-resistant tooling.

How to choose

Choose pure PTFE when chemical resistance, low friction or food / pharmaceutical suitability are paramount. Choose a filled grade when the part carries load or sees sliding wear. If stiffness and precision are needed and the chemical environment is not aggressive, POM or PEEK are often better.

Suitable PTFE machining services can be found or requested on the CNC Pasaulis marketplace.

Frequently asked questions

Are PTFE and Teflon the same?

Yes, Teflon is a widely used trade name for PTFE. Technical documents use the material name PTFE.

Why do PTFE part dimensions change?

PTFE expands strongly with heat, creeps under load and undergoes a phase transition at about 19 °C that changes volume by about 1 %. Machining and measuring must therefore be done at a stable temperature.

What temperature can PTFE withstand?

Continuous service is approximately −200 to +260 °C. Above about 400 °C the material begins to decompose and release toxic fumes.

What is bronze-filled PTFE used for?

It is used for loaded sliding parts such as guide rings in hydraulic cylinders, because it creeps less and wears more slowly than pure PTFE.

How should PTFE be clamped for machining?

Gently and evenly, for example with wide soft jaws or a vacuum table. Excessive clamping force deforms the material and changes dimensions after release.

Looking for someone to do this job? Find a manufacturer on the marketplace or post a request.

Services offered I need a service