Structural Steel S235 and S355: Properties and Machining
Updated
S235 and S355 are non-alloy structural steels to EN 10025-2, where the number is the minimum yield strength in MPa. They are inexpensive, easy to weld and moderately easy to machine, making them a common choice for frames, plates, brackets and welded assemblies, but they cannot be through-hardened.
Structural steels S235 and S355 are hot-rolled non-alloy steels specified in EN 10025-2, where the number in the grade indicates the minimum yield strength (ReH) in megapascals for thicknesses up to 16 mm. They are the most widely used steel grades in machine building, steel structures and CNC-machined plate parts.
Designation and equivalents
The full designation consists of the letter S (structural steel), the yield strength and an impact toughness class: JR (tested at +20 °C), J0 (0 °C), J2 (−20 °C) and K2 (−20 °C with higher energy). For example, S355J2+N is normalized or normalized-rolled steel with impact energy verified at −20 °C. Material numbers per EN 10027-2 are S235JR – 1.0038, S235J2 – 1.0117, S355JR – 1.0045 and S355J2 – 1.0577. Older DIN drawings use St37-2 (≈ S235JR) and St52-3 (≈ S355J2). The closest ASTM grades are A36 (≈ S235) and A572 Grade 50 (≈ S355), but these are only approximate equivalents – chemical composition limits and testing requirements differ. See material designation equivalents for more.
Key properties
| Property | S235JR | S355J2 |
|---|---|---|
| Density | ≈ 7.85 g/cm³ | ≈ 7.85 g/cm³ |
| Min. yield strength ReH (t ≤ 16 mm) | 235 MPa | 355 MPa |
| Tensile strength Rm (3–100 mm) | 360–510 MPa | 470–630 MPa |
| Typical hardness | ≈ 100–150 HB | ≈ 140–190 HB |
| Carbon content (max.) | ≈ 0.17–0.20 % | ≈ 0.20–0.24 % |
| Machinability | fair, prone to smearing | fair to good |
Hardness values are indicative only, as EN 10025-2 does not specify hardness; they depend on rolling condition and thickness. For conversion between scales see hardness scales.
Machinability
In the ISO 513 classification these steels belong to group P (see ISO material groups). Because of its low carbon content and high ductility, S235 is soft and gummy: at low cutting speeds a built-up edge forms on the cutting edge, the surface becomes torn and chips are long and hard to break. S355, with higher strength and manganese content, usually cuts more cleanly and gives a better surface finish.
Typical starting values for coated carbide tools (the tool manufacturer's data takes priority):
| Operation | Cutting speed Vc | Feed |
|---|---|---|
| Milling with an end mill | 150–250 m/min | fz ≈ 0.05–0.15 mm |
| Turning (roughing) | 180–280 m/min | f ≈ 0.2–0.4 mm/rev |
| Drilling with a carbide drill | 80–120 m/min | f ≈ 0.1–0.25 mm/rev |
For calculating spindle speed and feed rate see cutting speed and RPM and feed per tooth.
Practical tips
- Do not cut too slowly. Low cutting speed and too small a feed promote built-up edge; a higher Vc and adequate fz usually improve the surface.
- Use sharp geometry. Positive rake inserts and end mills with polished flutes reduce smearing.
- Control the chip. In turning, choose inserts with a chipbreaker designed for group P and your feed range.
- Account for residual stress. Hot-rolled plate contains residual stresses; removing a lot of material from one side can cause distortion. Machine symmetrically, leave stock, and take the finishing pass after releasing the clamps.
- Get under the mill scale. Rolling scale is abrasive – take the first pass deep enough that the cutting edge works below the scale layer.
- Corrosion protection. These steels rust, so parts need painting, galvanizing or oiling.
Typical uses
Machine and equipment frames, base plates, brackets, flanges, mounting plates, welded assemblies and building structures. S355 is chosen when higher load capacity or thinner sections are required. If a part needs hardening or higher surface hardness, carbon steel C45 or alloy steel 42CrMo4 is a better choice.
How to choose between S235 and S355
- If cost, weldability and bending matter most and loads are modest – S235JR.
- If higher strength, lower weight or service at low temperature is needed – S355J2.
- If a clean milled surface is important – S355 often machines better than S235.
- If the part must be hardened, neither grade is suitable: the carbon content is too low.
Milling and turning services for structural steel parts can be found or requested on the CNC Pasaulis marketplace.
Frequently asked questions
Can S235 or S355 be hardened?
Not by conventional quenching. With carbon up to about 0.2 %, these steels hardly respond; case hardening is possible, but dedicated case-hardening steels are normally used for that.
What is the difference between S355JR and S355J2?
Both have the same yield strength, but J2 guarantees impact toughness at −20 °C, whereas JR is tested only at +20 °C. J2 is recommended for welded structures and low-temperature service.
Why does S235 give a rough surface when milled?
The soft, ductile steel tends to build up on the cutting edge. Higher cutting speed, sharp positive-rake tools and coolant help.
What are the equivalents of St37 and St52?
The old DIN grade St37-2 roughly corresponds to S235JR and St52-3 to S355J2 under EN 10025-2.
Why does a part warp after milling?
Hot-rolled plate contains residual stresses that redistribute when material is removed. Machining symmetrically and leaving stock for a finishing pass reduces distortion.